summary:This paper describes the preparation of a powder coating for fire-fighting pipelines that fully meets the performance requirements of the standard "Automatic Sprinkler Systems Part 20: Coated Steel Pipes" through screening of raw materials such as film-forming resins, additives, pigments and fillers, as well as research on powder coating production processes and fire-fighting pipeline plastic coating processes.

Of particular note is that this paper solves the problem of hot water resistance of the coating after applying plastic powder coating to galvanized pipes.

1. Frontier
   
Ordinary fire-fighting galvanized pipes and fittings have poor performance in terms of corrosion resistance, scale prevention, and antibacterial properties. Combined with the characteristics of fire-fighting water—long-term stasis and sudden emergency use—these factors lead to numerous problems in practical applications.

First, due to the poor corrosion resistance of galvanized steel pipes, the inner surface of the pipes is prone to rusting when exposed to water for a long time, and the rust layer can easily clog the nozzles after it falls off.

Secondly, scale buildup on the inner surface of the pipe can easily reduce the inner diameter of the pipe or cause blockage, reducing or even preventing the delivery of water or gas, thus affecting the actual performance.

Furthermore, and most importantly, if the above-mentioned situation occurs during fire rescue operations, delaying rescue efforts, the consequences will be unimaginable; the existence of the above-mentioned defects results in a shorter service life for galvanized pipes, generally only 7-8 years.

In addition, zinc vapor in the hot-dip galvanizing process can easily cause zinc poisoning to operators, and the splashing of zinc ash and molten zinc during high-temperature hot-dip galvanizing can easily burn operators. Furthermore, hot-dip galvanizing causes serious environmental pollution.
   
To avoid the above situation, many fire protection pipe manufacturers have switched to using plastic-coated steel pipes instead of the previously commonly used galvanized pipes, such as coating the outer surface of the steel pipe with a layer of powder coating.

The inner surface of the plastic-coated steel pipe is smooth, resulting in low fluid resistance, increased flow rate, and no scaling or microbial growth. This ensures optimal flow rate and performance, while also being energy-efficient and environmentally friendly.

Furthermore, plastic-coated steel pipes have excellent resistance to chemical corrosion, water, solvents, proteins, and high-expansion foam extinguishing agents. They can solve the corrosion problems of fire-fighting pipelines caused by water transportation, burial, and acids, alkalis, and salts, and will greatly improve the service life of fire-fighting pipelines, with a service life of more than 50 years.

In addition, the powder coating for plastic-coated steel pipes does not contain organic solvents that pose health hazards to coating production and painting personnel;

Furthermore, powder coating is applied in a closed system, and spilled powder coating can be recycled and reused, with a coating utilization rate of over 98%, which can save a large amount of limited human resources.

Furthermore, most foreign building fire protection water supply systems use copper and stainless steel pipes. Due to the high cost of copper and stainless steel pipes, they are rarely used in engineering practice in my country.

Currently, fire water supply pipes for automatic sprinkler systems in China generally use galvanized steel pipes or galvanized seamless steel pipes. However, due to the poor corrosion resistance, scale prevention, and antibacterial properties of galvanized pipes, some fire pipe manufacturers have begun to produce plastic-coated fire pipes.

Comparing the prices of galvanized pipes and plastic-coated steel pipes: galvanized pipes are approximately 5,000 to 6,000 yuan per ton; black iron pipes are approximately 3,380 yuan per ton; and powder coating for plastic-coated steel pipes is 35,000 to 40,000 yuan per ton.

Since 50kg of powder coating can coat approximately 1 ton of black iron pipe, the price of coated steel pipe is approximately 5130-5380 yuan/ton.

From a cost perspective alone, galvanized pipes and plastic-coated steel pipes are similar. However, since the service life of plastic-coated steel pipes is 6-7 times that of galvanized pipes, considering both the cost and service life, plastic-coated steel pipes are much cheaper than galvanized pipes.
   
Previously, there were no standards for plastic-coated fire-fighting pipes. Factory inspections were mostly carried out in accordance with the requirements of the People's Republic of China Urban Construction Industry Standard "Water Supply Plastic-Coated Composite Steel Pipe" (CJ/T 120-2008). There were no special requirements for the powder coating used for plastic coating. Therefore, there were many types of powder coatings available for fire-fighting pipe manufacturers to choose from.

However, the Tianjin Fire Research Institute of the Ministry of Public Security recently formulated a new standard, "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes," which, compared to "Water Supply Plastic-Coated Composite Steel Pipes" (CJ/T 120-2008), adds the following indicators:

(1) Vacuum resistance: The length of the pipe section specimen is (500±50) mm. Use appropriate measures to block the inlet and outlet of the pipe, gradually increase the negative pressure from the inlet to 660 mmHg, and maintain it for 1 min. After the test, check that the inner coating has not peeled off.

(2) High temperature resistance: The length of the pipe section specimen is (100±10) mm. The specimen is placed in a constant temperature chamber, heated to (300±5)℃, and kept at the temperature for 1 h. Then it is taken out and cooled to room temperature naturally. After the test, the specimen is taken out and the inner coating is checked (the appearance color may darken or become dull). There should be no peeling, bulging, cracking, peeling or damage.

(3) Low temperature resistance: The length of the pipe section specimen is (100±10) mm. The specimen is placed in a low temperature chamber, cooled to (-30±2)℃, and kept at a constant temperature for 1 h. Then it is taken out and placed in an environment with a temperature of (20±5)℃ for (4~7) h.

After the test cycle is completed, take out the specimen and check that the inner coating is free from peeling or damage. Then, conduct an adhesion test according to the provisions of 7.4.2 in CJ/T120-2008. The adhesion of the coating should be grade 1 to 3.


(4) Pressure cycling: The length of the pipe section specimen is (500±50) mm. Use appropriate measures to block the inlet and outlet of the pipe and connect it to the water pressure supply system. Fill with water to remove air, and then conduct 3000 alternating water pressure tests from (0.4±0.1) MPa to MPa. The cycle of each test is no more than 2 s.



After the test, check that the inner coating is free from peeling or damage. Then, conduct an adhesion test according to the provisions of 7.4.2 in CJ/T120-2008. The adhesion of the coating should be grade 1 to 3.

(5) Temperature cycling: The length of the pipe section specimen is (500±50) mm. The specimen is placed under each temperature condition for 24 h in the following order: (50±2)℃; (-10 ±2)℃; (50±2)℃; (-10 ±2)℃; (50±2)℃; (-10 ±2)℃.

After the test, the specimen was placed in an environment with a temperature of (20±5) ℃ for 24 h. The inner coating was checked and found to be free of peeling or damage. Then, the adhesion test was carried out according to the provisions of 7.4.2 in CJ/T120-2008. The adhesion of the coating should be grade 1 to 3.

(6) Resistance to water aging: The length of the pipe section specimen is about 100 mm. The exposed ends of the pipe section should be treated with appropriate anti-corrosion measures. The pipe section is immersed in distilled water at (70±2)℃ for 30 days. After the test, it is taken out and naturally cooled to room temperature. The inner coating of the specimen should be checked and there should be no peeling or damage.
   
Because the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes" has added the above six indicators according to the actual use of fire protection pipelines, fire protection pipeline manufacturers have begun to conduct a large number of tests to screen powder coatings for plastic-coated steel pipes.

However, existing powder coatings on the market cannot meet the stringent requirements of the standard "Automatic Sprinkler Systems Part 20: Coated Steel Pipes". Therefore, many powder coating manufacturers have begun to develop new powder coatings that can meet the requirements of "Automatic Sprinkler Systems Part 20: Coated Steel Pipes".

2. Research on the Formulation of Powder Coating for Fire Protection Pipelines

2.1 Selection of film-forming resin
   
Powder coatings made with epoxy resin as the matrix have the following advantages:

(1) Powder coatings have low melt viscosity and good leveling properties; no by-products are produced during the curing reaction, the coating has good smoothness, and it is not easy to produce defects such as pinholes and craters.

(2) Since epoxy resin molecules have hydroxyl groups, they have good adhesion to substrates such as metals and generally do not require a primer.

(3) The coating has high hardness and good scratch resistance.

(4) The epoxy resin structure contains a bisphenol A backbone and a flexible ether chain, resulting in good physical and mechanical properties of the coating film.

(5) Powder coatings have good color matching and powder mixing properties, and a wide range of curing agent varieties to choose from.

(6) Powder coatings have good coating adaptability and can be applied by electrostatic powder spraying, fluidized bed dip coating, flame spraying and air spraying.
   
Therefore, we chose epoxy resin as the main film-forming resin. Furthermore, epoxy resins used in powder coatings must meet the following conditions to obtain excellent coatings:

a. The resin base material must be reactive;
b. The resin softening point should be controlled between 85 and 95°C;
c. The molecular weight distribution of the resin should be narrow.
   
E-12 epoxy resin (also known as 604# or 664# epoxy resin) has a softening point between 85 and 95°C, moderate viscosity, and meets the above three conditions, so we chose E-12 epoxy resin.

2.2 Selection of curing agent
   
In addition to meeting the general requirements for curing agents used in powder coatings, curing agents for epoxy powder coatings should also possess active groups that can cross-link with reactive groups such as epoxy groups and hydroxyl groups in epoxy resins.

There are many types of curing agents that meet these conditions. Currently, the ones widely used in industrial production include dicyandiamide, substituted dicyandiamide, sebacate dihydrazide, acid anhydrides, imidazoles, cycloamidinides, as well as phenolic hydroxyl resins (also known as phenolic curing agents), polyester resins, and acrylic resins.

Because the reaction between phenolic hydroxyl resin and epoxy resin is an addition reaction, no volatile substances escape during film formation, and no pinholes or pores are generated. This makes it particularly suitable for coating workpieces requiring thick coating, such as valves and elbows in oil, natural gas, and tap water pipes, as well as irregularly shaped parts like fire-fighting equipment. Therefore, we choose phenolic hydroxyl resin as the epoxy resin curing agent.

2.3 Selection of film-forming aids

2.3.1 Leveling agent
Leveling agents are one of the most important additives in powder coatings. In powder coating formulations, leveling agents must be added when a smooth, even coating appearance is required.

The role of leveling agents is to form an extremely thin monolayer on the surface of the molten coating when the powder coating melts and flows, so as to provide uniform surface tension.

Leveling agents are divided into two main categories: one category can be called leveling accelerators, whose main function is to eliminate orange peel, but their effect on eliminating pinholes is relatively weak; the other category can be called wetting accelerators, whose main function is to eliminate pinholes, but they cannot eliminate orange peel.

Normally, leveling accelerators can be used alone, but in cases where pinholes are easily formed, both must be used in combination.

2.3.2 Degassing agent (degassing agent)
Degassing agents (de-gas agents) are additives used in the current process of powder coating melt flow and film formation to release air, moisture, and volatile substances such as small molecule compounds produced during the cross-linking and curing reaction of powder coating. They also help to promptly close the pinholes caused by the released small molecule compounds, thus preventing defects such as small pinholes or pig-hair pores in the coating film.

This additive is one of the most commonly used additives in powder coatings, and it must be added to powder coating formulations in general[2]. The degassing agent commonly used in powder coatings is benzoin, also known as diphenylethanol ketone (commonly known as benzoin).

2.3.3 Antioxidants
The standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes" has requirements for both high-temperature and low-temperature resistance of the coating after plastic coating. Epoxy resin that can withstand temperatures as low as -30℃ can meet the requirements, while powder coatings made solely from epoxy resin as a film resin do not meet the requirement of withstanding temperatures as high as 300℃.

Therefore, we need to select some antioxidants to improve the temperature resistance of the coating. Since antioxidant 1010 has a melting point of 110.0~125.0℃ and can be added during the product polymerization process, manufacturing, or final use, it has a wide range of applications, so antioxidant 1010 is selected when formulating the product.

2.4 Selection of pigments and fillers

2.4.1 Packing
Fillers are an important component in powder coating formulations. Except for transparent powder coatings, most powder coatings require fillers and are an indispensable part of the powder coating formulation.

Commonly used fillers in powder coatings include precipitated barium sulfate, barite powder, light calcium carbonate, heavy calcium carbonate, kaolin, talc powder, bentonite, precipitated silica, mica powder, quartz powder, and silica microparticles.
   
Because the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes" requires that the coating after plastic coating has high temperature resistance, some heat-resistant fillers, such as hollow glass microspheres and mica powder, should be selected in the powder coating formulation.

Hollow glass microspheres are thick-walled spherical bodies with good fluidity, a Mohs hardness of 5-7, and a temperature resistance of over 1400℃. Adding hollow glass microspheres can improve the hardness and heat resistance of coatings.

Mica powder has a temperature resistance of over 600℃, and its fine flaky crystalline structure can improve the density of the coating and prevent moisture penetration.

In addition to heat-resistant fillers, some precipitated barium sulfate also needs to be added to the formula. On the one hand, precipitated barium sulfate is relatively inexpensive, which can reduce the cost of powder coatings; on the other hand, precipitated barium sulfate can enhance the leveling and gloss retention of powder coatings and has good compatibility with all colorants.
   
In addition, since the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes" also requires that the coating after plastic coating can pass the impact resistance, flattening resistance and bending resistance tests, this requires that the coating after powder coating must have good flexibility.

To improve the flexibility of the coating, some functional fillers, such as nano-silica, need to be added to the powder coating formulation.

Adding nano-silica to epoxy resin-based powder coatings results in a structure completely different from epoxy powder coatings with added coarse-grained SiO2 (such as silica), which is generally added as a reinforcing agent.

It is mainly distributed in the middle of the polymer chain. Due to its severe lack of coordination, large specific surface area and lack of oxygen on the surface, nano-silica exhibits extremely strong activity and can easily bond with the oxygen in epoxy cyclic molecules, thereby increasing the intermolecular bonding force.

Meanwhile, some nano-silica particles are still distributed in the gaps of the polymer chains. Compared with coarse-grained SiO2 particles, they exhibit high flowability, which greatly improves the strength and toughness of epoxy powder coatings with added nano-silica.

In addition, the addition of nano-silica can improve the wear resistance and anti-aging properties of the coating, as well as improve the surface finish of the coating.

2.4.2 Pigments
Pigments play a crucial role in powder coating formulations by coloring the coating film and creating decorative effects; they are an indispensable component for colored powder coatings.

Because the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes" requires that the coating after plastic coating must be red and able to withstand high temperatures, red inorganic pigments or red organic pigments with good temperature resistance are selected.

2.5 Determine the powder coating formulation

图片

After a series of experiments, the grades and amounts of the above raw materials were selected. Taking into account the performance of the coating, the feasibility of making powder coatings, and the performance of the coating process, the formula of the powder coating for fire-fighting pipeline plastic coating was finally determined, as shown in Table 1.

3. Research on the production process of powder coatings for fire protection pipelines
   
The special powder coating for fire protection pipelines is produced by melt extrusion, and the process flow is shown in Figure 1.

图片

3.1 Premixing
   
To ensure uniform dispersion of the various raw materials in the powder coating formulation, the materials are accurately weighed according to the formulation and premixed before melt extrusion.

Currently, in the production of powder coatings using epoxy resin as the film-forming resin system, high-speed mixers are generally used for premixing. During the premixing process, controlling the mixing time is crucial. Too short a time results in uneven mixing.

If the mixing time is too long, the material is prone to clumping, and if the premixing is too fine, melt extrusion will be more difficult. Furthermore, when the mixing time is too long, the coating color of some powder coating varieties will also show obvious differences.

Therefore, the mixing time for each batch of the same type of powder coating must be controlled to be the same to ensure consistent product quality, such as the applied color. We generally set the mixing time to 6-8 minutes.

3.2 Melt Mixing
   
Premixed materials are only macroscopically homogeneous; to achieve microscopic or submicroscopic homogeneity, they must undergo melt mixing. In China, melt mixing often uses twin-screw extruders. These extruders, along with tablet coolers and crushers, form a three-in-one integrated system, typically controlled by the same control cabinet.
   
When using a twin-screw extruder for mixing, the following issues should be noted:

a. Feed particle size: Premixing that is too coarse or too fine will cause difficulties in extrusion. Therefore, an appropriate feed particle size should be selected.

b. Extruder heating temperature: Generally, extruders are divided into three to four sections according to the heating temperature, namely the feeding section, plasticizing section (melting section), homogenizing section (mixing section) and discharge section.

The feeding section has the lowest temperature, and the temperature at the feed port must be lower than the glass transition temperature of the resin used in powder coatings. This is to prevent the material from sticking to the feed port due to overheating (the cooling water in the feeding section is usually kept on).

The temperature of the homogenization (mixing) section should be 10-20°C higher than the softening point of the resin used in powder coatings; the temperature of the plasticizing (melting) section is slightly lower than that of the homogenization section, but much higher than that of the feeding section, and there is a large temperature gradient in the plasticizing section.

The temperature of the discharge section is higher than that of the previous sections, but the temperature of this section should not be set too high, otherwise the powder will undergo a chemical reaction in the extruder, or even gel solidify.

If some of the gelling agents are introduced into the powder coating product, it will affect the product quality, often becoming particles (or spots) in the coating film. For powder coatings with epoxy resin as the main film-forming resin, the discharge temperature is generally set to 95-100℃.

c. Cooling and Crushing: The extruded material is at a very high temperature and may still undergo chemical reactions, so it must be cooled as quickly as possible. Cooling and crushing generally uses a tablet press. The extruded hot material is rolled into flakes by cooling rollers, and then the flakes are cooled on a cooling belt by air cooling. Finally, the cooled flakes are crushed into particles suitable for pulverization.

3.3 Crushing and sieving
   
The material, after being melt-extruded and cooled and crushed, is further pulverized, classified, and sieved to obtain powder coating products. In the manufacturing process of powder coatings, the fine pulverizing, classifying, and sieving equipment is an inseparable, interconnected system.

The main equipment of this system includes an air classifier mill (ACM mill), a screw feeder, a cyclone separator, a sieve, a bag filter, a rotary valve (also called a discharge valve or air shut-off valve), an induced draft fan, and a pulse oscillator.

The material is fed from the screw feeder to the air classifier mill. After reaching a certain particle size through the internal crushing device, the coarse particles are repeatedly crushed due to the action of the internal classifier, while the fine particles enter the cyclone separator under the suction of the blower.

In the cyclone separator, due to the centrifugal force of the cyclone, the coarse powder moves downward and enters the sieving machine through the rotary valve (discharge valve), while the ultrafine powder coating enters the bag filter.

Due to the filtration effect of the filter bags, the ultrafine powder coating remains outside the bags, while only air passes through the bags and is released into the atmosphere.

The powder coating entering the powder screening machine is screened. The product passes through the screen, while the coarse powder does not. The coarse powder can be automatically re-entered into the crusher for further crushing.
   
The following two issues should be noted in the fine grinding and grading sieving processes.

a. Size of the air intake of the blower: If the air intake is too large, too much fine powder will be drawn into the bag filter, affecting the product yield of the powder coating; if the air intake is too small, the content of ultrafine powder coating in the powder coating product will be too high, affecting the dry powder flowability and powder application rate of the powder coating.

b. Screening: The mesh size of powder coatings for pipes should generally be controlled between 120 and 180 mesh. Too coarse, and it will affect leveling; too fine, and it will produce a lot of dust and have poor flowability.

In addition, considering the ease with which screens can break, screens should be replaced periodically after a certain quantity of powder coating products has been produced. It is best to use anti-static screens to prevent powder coating from adhering to the screen and affecting the sieving effect.

3.4 Finished Product Packaging
   
Because powder coatings are susceptible to moisture absorption, heat, and clumping under pressure during storage and transportation, they are generally packaged in polyethylene film bags, which are then tightly sealed and placed into cartons or tubes.

Each box typically weighs 20kg net. Finished powder coatings are best stored in a dry warehouse at a temperature below 30℃, away from fire and heat sources.

Users are also required to store powder coatings under the following conditions. Additionally, when stacking finished powder coatings, strictly control the stacking height to prevent excessive pressure that could damage the packaging and cause the powder coating to clump together.

3.5 Storage stability test of powder coating for fire protection pipelines
   
Following the method described in standard GB/T 21782.8-2008 "Powder Coatings Part 8: Evaluation of Storage Stability of Thermosetting Powder Coatings", the powder coating for fire-fighting pipeline coating was first passed through a 65-mesh sieve, and then the gelation time at 180°C was measured to be 25 seconds.

Five samples were sprayed with the powder coating, and the three better samples were selected and their gloss was measured using a 200, 600, and 850 three-angle gloss meter. The results were: 34.9 gloss at 200 angle, 69.6 gloss at 600 angle, and 81.4 gloss at 850 angle.
   
Weigh three 100g samples and place them in separate glass test tubes. Hold the test tubes vertically and tap the bottom of the tubes on a sturdy surface to ensure that the powder is not loosely packed.

Then, carefully place an aluminum foil disc, roughly the same size as the test tube, on the sample surface, and gently place a 100g standard load (we used a 100g steel ball instead in our test) on the disc.

Stopper the test tubes and seal them with tape to prevent water from getting in. Place the test tubes on a test tube rack and then put them in 40°C warm water.

Store the powder coating for 24 hours, 7 days, and 28 days respectively, following the steps described above. Then remove the stopper from the test tube, tap the bottom of the test tube gently, and observe whether the powder coating can flow freely. Pour the powder coating into a clean container and observe whether the powder coating becomes compacted or clumps together.

Results: The powder coatings stored for 24 hours and 7 days were still relatively loose and did not show any compaction or clumping. A small number of small clumps appeared in the powder coatings stored for 28 days, but these clumps could be easily crushed by hand and did not affect the coating.
   
The gelation time of powder coating samples for fire-fighting pipeline plastic coating after 24h, 7d and 28d of storage was measured again. The results showed that the gelation time after 24h and 7d of storage was 25s, and the gelation time after 28d was 24s.

The gloss of the sample was also basically unchanged when it was coated again with the stored powder coating. This indicates that the powder coating for fire protection pipelines has good storage stability.

4. Research on Plastic Coating Technology for Fire Protection Pipelines

4.1 Research on Coating Methods
   
Coating methods can be divided into cold coating and hot melt coating. Cold coating generally uses electrostatic spraying and is suitable for workpieces that require a thin coating.

Because the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes" requires a coating thickness greater than 300 μm, cold coating is not applicable; only hot-melt coating can be used. Depending on the powder application method, hot-melt coating can be divided into thermal spraying, fluidized bed coating, and vacuum coating, among others.

4.1.1 Thermal spraying method
Thermal spraying involves preheating the workpiece to above the melting temperature of epoxy resin, then spraying powder coating onto the surface of the workpiece. The heat from the workpiece melts the powder, forming a smooth coating.

When spraying cylindrical containers or pipes, the workpiece should be rotated to ensure uniform powder distribution. The advantages of this method are simple equipment and convenient operation; currently, most steel pipe plastic coating in China uses this process.

4.1.2 Vacuum coating method
The method involves preheating the workpiece to a certain temperature, then creating a negative pressure inside the steel pipe to draw powder into the pipe, where it is evenly distributed on the inner wall of the pipe and melted into a smooth and flat coating.

This method involves simple production equipment, eliminates the need for reciprocating spraying, and boasts high production efficiency. It is applicable to steel pipes with a diameter of Dg100 or less, and is particularly suitable for small-diameter pipes where thermal spraying is difficult.

4.1.3 Fluidized Bed Method
Fluidized bed coating is suitable for simultaneous coating of the inner and outer walls of steel pipes. After the workpiece is fully preheated, it is immersed in the fluidized bed. Due to the heat, the powder can adhere to the substrate surface, resulting in a uniform coating after plasticization. To achieve sufficient thickness, the semi-plasticized workpiece can also be coated again using the fluidized bed method.

4.2 Study on the coating process

4.2.1 Surface treatment of the substrate
To obtain high-performance fire-fighting pipe coating products, the substrate must undergo surface treatment before coating. Surface treatment includes degreasing and rust removal.
   
Degreasing can be achieved through solvent degreasing, degreasing agent degreasing, and high-temperature combustion degreasing. High-temperature combustion degreasing is currently the most commonly used method.
   
Rust removal can be achieved using chemical and mechanical methods. Currently, phosphating is the primary chemical method. Mechanical methods mainly employ shot blasting or sandblasting. Sandblasting is currently the most widely used rust removal method. 4.2.2 Preheating
   
Except for cold spraying, regardless of the coating method used, the workpiece must be preheated before applying fire-fighting pipeline powder coating. Controlling the preheating temperature is crucial for successful application of fire-fighting pipeline powder coating.

The preheating temperature directly affects the flexibility and adhesion of the coating. During our experiments, we found that when the preheating temperature was set to 230℃ or higher, the coatings made with the same powder coating failed to meet the requirements of the standard "Automatic Sprinkler Systems Part 20: Coated Steel Pipes" in terms of impact resistance, flattening resistance, and bending resistance. Furthermore, after boiling in water, the adhesion barely reached level 3.

When the preheating temperature is set at or below 220℃, it can pass all the tests required in the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes".
   
To determine the preheating temperature range, we used a temperature point that decreased by 10°C every 10°C between 200°C and 130°C, and preheated at this temperature for 30 minutes. Then, the preheated pipe fittings were subjected to fluidized bed immersion coating and cured at 180°C for 30 minutes.

The plastic-coated pipe fittings were tested according to the requirements of the standard "Automatic Sprinkler Systems Part 20: Coated Steel Pipes", and all of them passed the test. In particular, the coating adhesion after boiling in water could even reach the Class 1 standard.
   
As shown in Table 2, this special powder coating for fire-fighting pipelines has a wide range of preheating temperatures and can achieve low-temperature preheating.

The coating, after preheating at 130℃ for 30 minutes, can pass all the tests required by the standard "Automatic Sprinkler Systems - Part 20: Coated Steel Pipes", which can greatly save energy consumption and reduce the cost of coating fire protection pipelines.

4.2.3 Application
After surface treatment and preheating, the pipe fittings can be powder coated. Regardless of the coating method used, the coating thickness must meet the requirements of the standard "Automatic Sprinkler Systems Part 20: Coated Steel Pipes" for nominal diameters DN≤65mm and coating thickness>300µm, and nominal diameters DN≥80mm and coating thickness>350µm.

4.2.4 Baking (Post-curing)
The performance of powder coatings for fire-fighting pipelines depends not only on the preheating temperature of the components, but also on the baking temperature and baking time.

After powder coating, the fire-fighting pipelines are placed in an oven for baking. If the baking temperature does not reach the specified temperature or the baking time does not reach the specified time, the cross-linking and curing of the coating will not be complete, which will affect the physical and mechanical properties of the coating.

Conversely, excessively high baking temperatures or prolonged baking times can cause discoloration or aging of the coating, affecting its various properties. Therefore, controlling the baking temperature and time during the curing process plays a crucial role in the coating's performance.

In actual production, different baking temperatures and baking times can be set according to the material, heat capacity and thickness of the object being coated. Generally, the baking temperature can be set between 160 and 200°C and the baking time is 10 to 30 minutes.

4.2.5 Cooling
Because the baking temperature of powder coating is relatively high, the temperature of the coated object is also relatively high when it comes out of the oven. After it comes out of the oven, it needs to be left for a certain period of time to cool down to a temperature that can be touched by hand (below 40℃).

There are two ways to cool the object being coated: forced cooling and natural cooling. Forced cooling uses cold air or cool water as a medium.

For materials with high latent heat, natural cooling is slow, resulting in a longer residence time on the production line, which necessitates a longer production line length. Therefore, forced cooling is preferable, as it shortens the coating production line and reduces coating time.
Note: Natural cooling mentioned here must not be followed by furnace cooling. If cooled in the furnace, the coating will be subjected to high-temperature aging for a long time, greatly shortening its lifespan.

4.3 Repair
   
If any defects or damage to the coating are found during the coating process or during the installation and use of coated products, they should be repaired promptly. If the coating suffers extensive damage, it can be removed by high-temperature burning, the substrate can be re-sandblasted, and then the same powder coating can be applied.

If the coating is only locally damaged, it can be repaired with epoxy repair adhesive, or it can be repaired by applying the same type of paint with local heating.

4.4 Touch-up coating
   
After the pipe fittings are preheated and coated with plastic, before they are put into the oven for baking, the quality inspectors will use a thickness gauge to measure whether the coating thickness meets the standard. If some areas are found to be thin, they can be marked with chalk. Then the coated pipes are put into the oven for curing. After curing for 10 to 15 minutes, the pipe fittings are taken out of the oven.

Reapply fire-fighting pipe powder coating to the areas marked with chalk, measure the coating thickness again, and then place the pipe fittings with acceptable thickness into an oven to continue curing for 15-20 minutes.

5. Performance Testing

5.1 Black iron pipes were selected as the base material.
   
The nominal diameter of fire-fighting pipes is required according to the standard "Automatic Sprinkler Systems Part 20: Coated Steel Pipes" (except for the bending test, the black iron pipes used in other tests are all DN=100mm).

The black iron pipe used in the bending test (DN=25mm) and the coating thickness (coating thickness is 300µm~400µm) are coated by thermal spraying, vacuum coating or fluidized bed method.

Then, according to the pipe fitting length required in this standard, samples for testing were cut from the plastic-coated fire pipe, and tests such as high temperature resistance, low temperature resistance, and adhesion were conducted according to the methods specified in the standard. The results are listed in Table 2.